  1. What is the specified rate of load application when testing concrete cylinders for compressive strength per ASTM C39?

    Answer: 35 ± 7 psi/s (0.25 ± 0.05 MPa/s)

    ASTM C39 specifies a constant loading rate of 35 ± 7 psi/s (0.25 ± 0.05 MPa/s) applied continuously and without shock throughout the test.

  2. Per ASTM C39, the bearing surfaces of cylinders must not depart from a plane by more than:

    Answer: 0.002 inch (0.050 mm)

    ASTM C39 requires bearing surfaces to be plane within 0.002 inch (0.050 mm), which is why capping or end grinding is typically required.

  3. Per ASTM C39, the diameter of a test cylinder used to calculate compressive strength must be the average of two measurements taken at:

    Answer: Right angles to each other at or near mid-height

    ASTM C39 requires diameter to be determined from two measurements at right angles to each other taken at or near mid-height of the specimen.

  4. According to ASTM C39, what age tolerance is permitted when testing concrete cylinders specified for a 28-day strength result?

    Answer: ± 20 hours

    ASTM C39 allows 28-day specimens to be tested within ± 20 hours of the specified test age.

  5. A cylinder measures 5.90 inches long and 3.00 inches in diameter, giving an L/D ratio of approximately 1.97. Which statement best describes how to handle this specimen per ASTM C39?

    Answer: Test and report the result with no correction since L/D is between 1.75 and 2.10

    ASTM C39 correction factors apply only when L/D is below 1.75; an L/D of 1.97 falls within the acceptable range and needs no correction.

  6. Which fracture pattern described in ASTM C39 is characterized by a well-formed cone on one end with no significant cracking through the capping material?

    Answer: Type 1 cone fracture

    A Type 1 fracture in ASTM C39 shows a well-formed cone on one or both ends with no cracks running through the caps, indicating good end conditions.

  7. When a test result is the average of two companion cylinders and one shows damage due to an improper cap (not a concrete deficiency), what should be done per ASTM C39?

    Answer: Discard the defective cylinder and report the companion result alone

    If a cylinder fails due to an obvious fabrication or capping defect, its result is discarded and the strength is reported from the valid companion cylinder.

  8. When consolidating a 6×12 inch concrete cylinder by rodding per ASTM C31, how many equal layers are required?

    Answer: Three layers

    ASTM C31 requires three equal layers when making 6×12 inch cylindrical specimens consolidated by rodding.

  9. What are the diameter and minimum length specified for the tamping rod used to consolidate standard concrete cylinder specimens per ASTM C31?

    Answer: 5/8-inch diameter, 24 inches long

    ASTM C31 specifies a tamping rod that is 5/8 inch (16 mm) in diameter and at least 24 inches (600 mm) long with a hemispherical tip.

  10. When using an internal vibrator to consolidate concrete cylinder specimens per ASTM C31, the vibrator diameter must not exceed what fraction of the mold diameter?

    Answer: One-fourth

    Per ASTM C31, the vibrator diameter shall not exceed one-fourth (1/4) of the diameter of the mold being filled.

  11. Per ASTM C31, what temperature range must be maintained during initial curing of concrete cylinder specimens in the field?

    Answer: 60–80°F (16–27°C)

    ASTM C31 requires specimens to be maintained between 60°F and 80°F (16°C and 27°C) during the initial curing period.

  12. After the top surface of a freshly cast cylinder is struck off, it must be finished so that it departs from a true plane by no more than:

    Answer: 1/16 inch (1.6 mm)

    The struck-off top surface must be finished level within 1/16 inch (1.6 mm) of a true plane per ASTM C31.

  13. Per ASTM C31, freshly cast concrete specimens must be protected from vibration, shock, and disturbance for a minimum of how long after molding?

    Answer: 24 hours

    Specimens must not be disturbed or transported for the first 24 hours after molding to prevent damage to the fresh concrete microstructure.

  14. When making concrete beam specimens for flexural strength testing per ASTM C31, which consolidation method is permitted when the measured slump is 3 inches (75 mm) or greater?

    Answer: Either rodding or internal vibration

    Per ASTM C31, when slump is 3 inches or more, consolidation may be achieved by either rodding or internal vibration.

  15. Per ASTM E4, how often must the testing machine used for compressive strength tests be verified for force-measurement accuracy?

    Answer: Every 12 months

    ASTM E4 requires testing machines to be verified at least every 12 months and whenever there is reason to question their accuracy.

  16. Unbonded neoprene pad caps used as an alternative to sulfur mortar for compressive strength testing must conform to which ASTM standard?

    Answer: ASTM C1231

    ASTM C1231 governs the use of unbonded neoprene pads in retaining rings as an alternative to sulfur mortar caps for testing concrete cylinders.

  17. Per ASTM C1231, which Shore A durometer hardness neoprene pad is specified for testing concrete with a design compressive strength up to 7,000 psi (50 MPa)?

    Answer: 50 durometer

    ASTM C1231 specifies 50 durometer neoprene pads for concrete with design strengths from 1,500 to 7,000 psi (10 to 50 MPa).

  18. Per ASTM C617, the maximum allowable thickness of a sulfur mortar cap on a test cylinder is:

    Answer: 3/16 inch (5 mm)

    ASTM C617 requires caps to be as thin as practicable and not exceed 3/16 inch (5 mm) in thickness.

  19. Which ASTM standard governs the flexural strength of concrete using a simple beam with third-point loading?

    Answer: ASTM C78

    ASTM C78 covers the determination of flexural strength (modulus of rupture) using a simple beam with third-point loading.

  20. A compressive testing machine must be accurate to within what percentage of the indicated load throughout the range being used, per ASTM E4?

    Answer: ± 1.0%

    ASTM E4 requires the force-indicating system to be accurate within ± 1% of the indicated load in the range being used.

Written and edited by , founder of Practice Test Geeks, with AI assistance. Exam facts are checked against the official sources linked below. Editorial policy

Sources & references

Exam facts on this page (fees, format, dates, passing scores) are checked against these official sources; the date is our last check. Editorial policy

  1. concrete.org — Exam dates, fees, retake fee, exam format, renewal, time limit, score validity, registration, retake policy, score release · verified Nov 2026
  2. acicentraltexas.starchapter.com — Fees, retake fee · verified Nov 2026
  3. prometric.com — Test delivery · verified Nov 2026